Specifications
Certification :
SDS
Place of Origin :
SHENZHEN
MOQ :
1KG
Payment Terms :
T/T
Supply Ability :
20kg/barrel
Delivery Time :
15
Price :
$10-$100
Property 7 :
Tensile Strength
Property 11 :
Temperature Resistance
Value 15 :
Mold making, gaskets, seals, medical devices, etc.
Value 1 :
Silicone
Property 14 :
Electrical Insulation
Property 5 :
Curing Method
Value 8 :
200-800%
Property 10 :
Specific Gravity
Value 10 :
1.1-1.5
Value 2 :
Liquid
Property 12 :
Chemical Resistance
Material :
silicone rubber
Value 4 :
Low to High
Value 5 :
Platinum-catalyzed
Value 13 :
Good
Description

Sprayable Self Adhesive Silicone Coating

KANGLIBANG® Silicone rubber

Product Description

KL-2680AB-50 ,Self adhesive silicone coating serves as heat fast curing sprayable version liquid silicone coating which adheres to the glass and silicone rubber products surface sparing from the use of silicone primers on the glass and silicone rubber products substrates.

Attention
1, The user should make changes based on spraying thickness and weather conditions (Temperature ,humidity).
2,The solvent is suppose to be blended solvent. xylol :Ethyl acetate:Cyclohexanone=80:15:5 or Tolune : Butanone =1: 1. too much water in the solvent will cause rough surfaces of liquid silicone coating.
3,The-ready-to-bond glass substrates should be washed clean till no dusts and oil dirts.
4 ,Check during spraying coating process , control the viscosity of the liquid silicone, make sure enough coating amount and get it cured completedly. 5,The spraying environment counts , It is advisable to adopt dust-free plant for production .Temperature controlled at 25~35℃. Humidity controlled at 25~50%. 6, The mixed liquid silicone must be used up in 6 hours , stop use the material when found viscosity increase or material get hardened

Processing

It is advisable to take KL-2680A and KL-2680B based on solid contents 25% (Weight ratio) KL-2680A:KL- 2680B:Solvent=100:100:200. 1,Take the KL-2680A and KL-2680B based on proportionated weight ratios and add the solvent lots by lots. mix evenly with 20-40 minutes . 2,Spray the mixed liquid silicone evenly on the glass and silicone surfaces.

3,When the spraying thickness is10μm ,bake with 150℃ for 2minutes. The baking time is determined by the baking temperature and spraying thickness. when the spraying thickness is 20μm, baking time should be increased to 3 minutes(Note : Data for reference only, please make change based on specifical situation )

Send your message to this supplier
Send Now

Self Adhesive Rtv 2 Liquid Silicone Rubber Liquid For Mould Making Coating

Ask Latest Price
Certification :
SDS
Place of Origin :
SHENZHEN
MOQ :
1KG
Payment Terms :
T/T
Supply Ability :
20kg/barrel
Delivery Time :
15
Contact Supplier
Self Adhesive Rtv 2 Liquid Silicone Rubber Liquid For Mould Making Coating

Shenzhen KangLiBang Technology Co., Ltd

Verified Supplier
2 Years
guangdong, shenzhen
Since 2010
Business Type :
Manufacturer
Total Annual :
5000000-10000000
Employee Number :
50~100
Certification Level :
Verified Supplier
Contact Supplier
Submit Requirement