1.4541 Weld-neck Flange according to EN 1092-1
Material No: 1.4541, 17248 / similar to AISI 321
Other PN and materials available on request
X6CrNiTi18-10 (1.4541) Chemical Composition
| Grade |
X6CrNiTi18-10 |
| Number |
1.4541 |
| Classification |
Austenitic stainless steel |
| Density |
7.9 g/cm³ |
Standards
- EN 10088-2:2005 Stainless steels - Technical delivery conditions for sheet/plate and strip
- EN 10088-3:2005 Stainless steels - Technical delivery conditions for semi-finished products, bars, rods, wire, sections and bright products
- EN 10028-7:2007 Flat products made of steels for pressure purposes - Stainless steels
- EN 10222-5:2000 Steel forgings for pressure purposes - Martensitic, austenitic and austenitic-ferritic stainless steels
- EN 10216-5:2014 Seamless steel tubes for pressure purposes - Stainless steel tubes
- EN 10217-7:2005 Welded steel tubes for pressure purposes - Stainless steel tubes
- EN 10296-2:2005 Welded circular steel tubes for mechanical and general engineering purposes - Stainless steel
- EN 10253-3:2008 Butt-welding pipe fittings - Wrought austenitic and austenitic-ferritic stainless steels
- EN 10253-4:2008 Butt-welding pipe fittings - Wrought austenitic and austenitic-ferritic stainless steels with inspection requirements
- EN 10272:2007 Stainless steel bars for pressure purposes
- EN 10263-5:2001 Steel rod, bars and wire for cold heading and cold extrusion - Stainless steels
- EN 10250-4:2000 Open steel die forgings for general engineering purposes - Stainless steels
- EN 10297-2:2005 Seamless circular steel tubes for mechanical and general engineering purposes - Stainless steel
- EN 10088-1:2005 Stainless steels - List of stainless steels
- EN 10088-5:2009 Stainless steels - Technical delivery conditions for construction purposes
- EN 10088-4:2009 Stainless steels - Technical delivery conditions for construction purposes
Chemical Composition % (EN 10088-2:2005)
| Element |
Content |
| C |
max 0.08 |
| Si |
max 1 |
| Mn |
max 2 |
| Ni |
9 - 12 |
| P |
max 0.045 |
| S |
max 0.015 |
| Cr |
17 - 19 |
| Ti |
max 0.7 |
Ti = 5 * C to 0.7
Particular ranges of sulphur content may provide improvement of particular properties. For machinability a controlled sulphur content of 0.015% to 0.030% is recommended and permitted. For weldability, a controlled sulphur content of 0.008% to 0.030% is recommended and permitted. For polishability, a controlled sulphur content of 0.015% max is recommended.
Elements not listed in this table shall not be intentionally added to the steel without the agreement of the purchaser except for finishing the cast.
Mechanical Properties
| Property |
Value |
| Rm - Tensile strength (+A) (MPa) |
500-720 |
| Rm - Tensile strength (+AT+C) (MPa) |
810-850 |
| Rm - Tensile strength (+AT) (MPa) |
460-730 |
| Rp0.2 0.2% proof strength (+A) (MPa) |
190-225 |
| Rp0.2 0.2% proof strength (+AT) (MPa) |
180-200 |
| KV - Impact energy transverse (+A) (J) |
+20°: 60, -196°: 60 |
| KV - Impact energy longitudinal (+A) (J) |
+20°: 100 |
| A - Min. elongation at fracture (+A) (%) |
30-40 |
| A - Min. elongation at fracture longitudinal (+AT) (%) |
35 |
| Nominal diameter (mm) |
2 - 50 |
| Z - Reduction in cross section on fracture (%) |
60-65 |
| Brinell hardness (+A) (HB) |
215 |
| Brinell hardness (+AT) (HB) |
210 |
Properties
Resistance to intergranular corrosion: in the delivery condition - yes; in the sensitized condition - yes
Steel shall not be applied at a metal temperature lower than -196°C
Equivalent Grades
Warning! Only for reference
| EU EN |
USA |
Germany DIN,WNr |
Japan JIS |
France AFNOR |
| X6CrNiTi18-10 |
321 |
X10CrNiTi18-9 X6CrNiTi18-10 |
SUS321 |
Z6CNT18-10 |
| England BS |
Italy UNI |
China GB |
Sweden SS |
Poland PN |
| 321S31 |
X6CrNiTi18-11 |
0Cr18Ni10Ti 1Cr18Ni11Ti H0Cr20Ni10Ti |
2337 |
0H18N10T 1H18N9T |
| Czechia CSN |
Finland SFS |
Austria ONORM |
Russia GOST |
|
17247 17248 |
731 |
X6CrNiTi18-10S |
08KH18N10T 08KH18N12T 12KH18N10T |
|